Cause analysis and solution for boiler high-temperature superheater tube bursting during 600MW supercritical unit startup commissioning;
600MW机组锅炉高温过热器爆管原因分析与处理
2.
Through comprehensive stress calculation of outlet header of high-temperature superheater,the stress defects during operation are found out,and shortages in boiler design are pointed out,at the same time,and the ultimate causes of crack between header and snake tubes are found.
通过对高温过热器出口联箱进行综合应力计算,查明设备运行过程中存在的应力缺陷,指出了锅炉设计中存在的不足,同时也找出了联箱与蛇形管根部开裂的根本原因。
3.
By the physico-chemical testing and analysis on the rupture and leakage failure of high-temperature superheater pipe of No.
对黄桷庄电厂22号炉高温过热器管爆漏失效进行了理化试验、分析,找到了引起锅炉失效的主要原因是超负荷运行,造成过热器处严重结焦,从而引起管子冲蚀、低温热腐蚀。
3) high temperature superheater
高温过热器
1.
Serious coking and ash depositions,that occurred in the high temperature superheater zone of a certain 220 t/h high pressure boiler,are being analyzed,showing that the main causes are: low melting point of the coal ash,too low a feed water temperature as well as soot-blower service defaults.
对某220 t/h高压锅炉发生的高温过热器区域严重结焦积灰堵塞现象进行了分析,主要原因是煤质灰熔点低、给水温度偏低和吹灰器未能正常投入。
2.
With the aid of scanning electron microscope(SEM) and X-ray diffractometer(XRD),an analysis is performed on scales formed on inner walls of G102 steel high temperature superheater tubes.
利用扫描电镜(SEM)及X射线衍射仪(XRD)对G102钢高温过热器管内产生的氧化皮进行分析。
3.
The reason of DG410/100-2 boiler high temperature superheater tube rupture are analyzed,the contradiction between keeping nomal main steam temperature and high temperature heat surface overheating,which is created after a nomal boiler changed into a peak shaving boiler are expounded.
分析了DG410/100-2型锅炉高温过热器爆管的原因,重点对带基本负荷机组改调峰机组后锅炉出现的保持正常主汽温度与高温受热面超温的矛盾作了阐述,从检修与运行两方面对预防措施进行了探讨。
4) superheater
[英][,sju:pə'hi:tə] [美][,supɚ'hitɚ]
高温过热器
1.
The failed superheater tube of a supercritical boiler in a power plant was studied by means of macrofractographic and metallographic examination,chemical composition analysis and mechanical property testing.
针对某电厂超临界锅炉高温过热器爆管的情况,通过爆口宏观分析、化学成分分析、金相分析以及爆口附近管段的力学性能测试,从该管段不同位置金相组织呈现的条状分布σ相,认定高温过热器长期超温。
5) HT superheater
高温过热器
1.
At present the conventional arrangement mode is widely used for HT superheaters of HT HP CFB boilers.
目前 ,高温、高压循环流化床锅炉高温过热器都采用常规布置方式 ,高温过热器上部受热面的材料必须采用SA2 13-T9l,它价格昂贵、加工工艺复杂 ,使高温过热器的造价较高。
6) high temperature superheater pipe
高温过热器管
1.
Through the comparison & analysis of high temperature superheater pipe explosion happened in 1973 and 2005,combined with site condition and test analysis,it is showed that sulfur corrosion is the main reason to result in the damage of high temperature superheater pipe under some special condition.
通过对某发电厂高温过热器管1973年和2005年两次爆管原因对比分析,结合现场情况及大量试验分析,说明硫腐蚀是高温过热器管在某种特殊情况下损坏的主要原因,并提出防范措施,对今后锅炉安全经济运行提出了相应的建议。
补充资料:动力机械:过热器
锅炉中将蒸汽从饱和温度进一步加热至过热温度的部件﹐又称蒸汽过热器。大部分工业锅炉不装设过热器﹐因为许多工业生产流程和生活设施只需要饱和蒸汽。在电站﹑机车和船用锅炉中﹐为了提高整个蒸汽动力装置的循环热效率﹐一般都装有过热器。采用过热蒸汽可以减少汽轮机排汽中的含水率。过热蒸汽温度的高低取决于锅炉的压力﹑蒸发量﹑钢材的耐高温性能以及燃料与钢材的比价等因素﹐对电站锅炉来说﹐4兆帕的锅炉一般为450℃左右﹔10兆帕以上的锅炉为540~570℃。少数电站锅炉也有采用更高过热汽温的(甚至可达650℃)。 类型和特点 过热器按传热方式可分为对流式﹑辐射式和半辐射式﹔按结构特点可分为蛇形管式﹑屏式﹑墙式和包墙式。它们都由若干根并联管子和进出口集箱组成。管子的外径一般为30~60毫米。对流式过热器最为常用﹐采用蛇形管式。它具有比较密集的管组﹐布置在 450~1000℃烟气温度的烟道中﹐受烟气的横向和纵向冲刷。烟气主要以对流的方式将热量传递给管子﹐也有一部分辐射吸热量。屏式过热器由多片管屏组成﹐布置在炉膛内上部或出口处﹐属于辐射或半辐射式过热器。前者吸收炉膛火焰的辐射热﹐后者还吸收一部分对流热量。在10兆帕以上的电站锅炉中﹐一般都兼用屏式和蛇形管式两种过热器﹐以增加吸热量。敷在炉膛内壁上的墙式过热器为辐射式过热器﹐较少采用。包墙式过热器用在大容量的电站锅炉中构成炉顶和对流烟道的壁面﹐外面敷以绝热材料组成轻型炉墙。图 过热器布置图 为几种过热器的布置。装有过热器的小容量工业锅炉一般只用单级管组的对流式过热器即能满足要求。 性能 锅炉运行工况的变化﹐例如负荷高低﹑燃料变化﹑燃烧工况变动等﹐都对过热器出口汽温有影响﹐所以在电站锅炉中都有调节锅炉出口汽温使其稳定在规定值的手段。常用手段有﹕ 用喷水式或表面式减温器直接调节汽温﹔ 用摆动燃烧器改变炉膛出口烟气温度﹔ 用烟气再循环调节过热器吸热量(见锅炉汽温调节)。锅炉负荷升高时﹐对流式过热器的进出口蒸汽温度升高值增大﹐辐射式过热器的温度升高值减小。若将对流式﹑辐射式和半辐射式过热器合理组合配置﹐则可在负荷﹑燃烧工况等变化时使出口汽温变化较小。过热器管组中各并联管子的吸热量和蒸汽流量在运行中都会有差别。为避免个别管子中温度过高﹐在大型锅炉中把过热器分成若干管组﹐用炉外的集箱对各管组蒸汽进行混合并用导汽管使各管组换位﹐以避免各管间出现过大的温度差。